Leave Your Message
Nickel Alloy GH4169/N07718 - Waxqabadka Sare ee Superalloy ee Xaaladaha Ba'an

Taxanaha Superalloy

Nickel Alloy GH4169/N07718, oo loo yaqaan Inconel 718, waa wax qabad heer sare ah oo loogu talagalay xaalado aad u daran. Daawaynta nikkel-chromium waxay caan ku tahay xooggeeda gaarka ah, iska caabbinta daxalka, iyo iska caabinta oksaydhka ee heerkul sare. Muujinaya xajinta sare, gurguurta, iyo xoogga dillaaca, GH4169/N07718 waxay ku habboon tahay codsiyada hawada, tamarta, iyo warshadaha saliidda iyo gaasta. Quruxdeeda cajiibka ah iyo kartida ay ku ilaalinayso guryaha farsamada heerkulka ilaa 1300°F (700°C) ayaa ka dhigaysa doorasho la isku halayn karo oo loo baahan yahay deegaan. Haddii loo isticmaalo marawaxadaha gaaska, matoorada diyaaradaha, ama qaybaha cadaadiska sare leh, Nickel Alloy GH4169/N07718 waxay hubisaa adkeysiga iyo hufnaanta codsiyada ugu adag.

    CUSBOONAYSIINTA Kiimikada

    SPACE

    %

    Gudaha

    Cr

    Fe

    Waayo

    Nb

    Co

    C

    Mn

    Iyo

    S

    leh

    Al

    ee

    P

    B

    GH4169
    N07718

    MIN

    50

    17

    dheelitirnaan

    2.8

    4.75

    -

    -

    -

    -

    -

    -

    0.2

    0.65

    -

    -

    MAX

    55

    21

    dheelitirnaan

    3.3

    5.5

    1

    0.08

    0.35

    0.35

    0.015

    0.3

    0.8

    1.15

    0.015

    0.06

    Guryaha Jirka

    cufnaanta

    Alloy state

    xoog adkaysi

    xoog dhalid

    Dheeraynta

    Dheeraynta

     

    N/mm2

    Rp0.2 N/mm2

    A5%

    HB

    8.24g/cm

    Daawaynta xal adag

    ≥965

    ≥550

    ≥30%

    ≤363

    Xalka adag + gabowga

    ≥1275

    ≥1034

    ≥12%

    ≥331

    HEERKA FULINTA

    PRODUCT

    Heerka ASTM

    Heerka ASME

    Xaashida, saxan, xariijin

    B670

    SB670

    Dhuumaha&tubo aan cillad lahayn

    B983

    -

    tuubo welded & tuubo

    -

    -

    Bar, Keega

    B637

    SB637

    Been abuurasho

    B670

    SB670

    Silig

    -

    -

    MUUQAALKA badeecada

    1.fudud mashiin. 2. Xoog adag oo xoog leh, xoog daal, xoog gurguurta iyo xoog jaban oo ah 700°C. 3. iska caabbinta oksaydhka sare ee 1000 ° C. 4. Halabuurka kiimikada deggan heerkulka hooseeya. 5. weldability wanaagsan.

    Codsiga alaabta

    Sababo la xiriira xoogga heerkulka sare iyo iska caabin daxalka aad u fiican at 700 ℃, processing fudud 718 waxaa si ballaaran loo isticmaali karaa in noocyo kala duwan oo waqti-dalbashada sare.

    Bandhiga Alaabta

    • GH44 (16)qn6
    • GH44 (17)rf
    • GH44 (26)j5g